Three settings on a braiding line are not three settings. Pitch, spindle speed and haul-off are one decision expressed three ways, and the density of the finished braid along its entire length is the record of whether they agreed. Change any one of them alone and the roll comes off either uniformly open or uniformly over-packed — a fault that is impossible to see station by station, because every crossing in it is individually correct.
This article defines pitch and braid angle precisely enough to be set, records the relationship between them that the process card depends on, and gives the two shop-floor measurements that let you verify on a finished braid what the settings claimed. It is the pitch and angle companion to the braiding process article, which covers the twelve stations the setting sits inside.
Pitch: the Axial Advance per Interlacement Cycle
Pitch is the axial distance the braid advances during one interlacement cycle — one pass in which the carriers cross at the braiding point. It is not a property of the yarn and it is not a property of the deck. It is the ratio of the two speeds the machine is running at:
pitch = haul-off (take-up) speed ÷ interlacement cycles per minute
Read off the shop floor, that is why the process card lists spindle speed and haul-off speed as a pair. The take-up decides how much braid leaves per unit time; the carrier motion decides how many interlacement cycles put material into it per unit time. Change the take-up alone and the pitch changes in direct proportion, and every metre of the run is affected equally.
Two further consequences follow from the same expression, and both catch people out. First, spindle speed has two different meanings on braiding equipment, and the one that matters here is the carrier motion. A maypole braider's figure describes the carrier motion of the whole machine — typically 300–800 rpm, above 1,200 rpm on high-speed machines — while a square braiding machine quotes its rotating spindle, for example 16 min⁻¹ on a BZ-32 or 25 rpm on a 336-series host. (industry reference) Quoting one as the other changes the pitch calculation by more than an order of magnitude. Second, "speed" alone is never a specification: the pair has to travel together, exactly as the process card records it.
Braid Angle: the Same Setting, Seen from Outside
Pitch is what the operator sets. Braid angle is what the customer sees. The two describe the same geometry from different directions, and the bridge between them is the circumference of the product.
A yarn leaving the braiding point does not travel straight along the braid. It wraps the tube helically, and one complete wrap carries it once around the circumference — a distance of 2πR for a braid of radius R — while the braid advances along its axis by the lead, the advance per full wrap. The braid angle α, measured between the yarn and the braid's axis, follows from that right-angle relationship:
tan α = circumference ÷ lead = 2πR ÷ lead
For a given machine and construction the number of interlacement cycles inside one full wrap is fixed by the deck, so lead and pitch differ only by a constant factor: for a given product, doubling the pitch doubles the lead, and the braid angle moves toward the axis. A plain, closed braid angle on a finished packing sits close to 45°; that is the point at which the lead equals the circumference (lead = 2πR), the yarns lying at 45° to the axis with the load sharing evenly between the axial and the hoop direction.
Note what the expression does when the diameter changes. At a fixed lead, a larger braid has a larger circumference, so tan α rises and the angle opens toward the transverse. The consequence is the single most useful fact in this article:
The same machine setting produces a steeper braid angle on a larger product and a flatter one on a smaller product. Setting a machine up on Ø6 and then running Ø20 without touching the process card does not reproduce the braid the customer approved — it reproduces the same pitch on a bigger circumference, which is a different braid angle. To hold the angle constant when the diameter changes, the lead has to change in proportion to the diameter, which means the take-up has to change with it.
Coverage: Why Pitch Is Also a Sealing Property
Pitch does not only tilt the yarns; it decides how much yarn is packed into a metre of product. Shorten the pitch at a fixed carrier count and more yarn ends are laid into every unit length: coverage rises, the braid closes, the surface firms up, and the material content per metre rises with it. Lengthen the pitch and the same yarns are spread over more length — an open, more flexible, lighter braid with visible gaps between yarns.
That is why coverage cannot be discussed apart from carrier count. Carrier count sets how many yarn ends are available per interlacement cycle (see the braid structure article in this series); pitch sets how much length each cycle is stretched over. The pair together decide the cover factor — the proportion of the surface actually occupied by yarn — and the cover factor is the real specification behind phrases like "tightly braided" or "open braid".
| Setting | Direction of change | What rises | What is given up |
|---|---|---|---|
| Pitch | Longer pitch (faster take-up, same spindle speed) | Output per hour, flexibility, braid angle measured from the axis falls | Coverage, density, sealing performance, tensile per unit length |
| Pitch | Shorter pitch (slower take-up, same spindle speed) | Coverage, density, surface tightness, sealing performance | Output, flexibility, yarn consumption per metre rises |
| Carrier count | More carriers | Coverage and strength at a given pitch; yarn consumption | Deck size, footprint, the ability to close around small sections |
Measuring Pitch and Angle on a Finished Braid
Both parameters are verifiable with what is on the bench, which is the point of setting them deliberately rather than adjusting until it looks right. (field practice)
Pitch. Lay a length of braid flat and straight on a lit surface. Find a feature that repeats — the point at which the diamond pattern returns to the same phase. Mark across a convenient number of repetitions, measure the marked span, and divide. Measuring over ten repetitions rather than one removes almost all of the reading error, and the result is a number that can be written on the record and compared with the process card.
Braid angle. Place a straight edge along the axis of the braid and read the angle of a single visible yarn against it, or read it from the diamond that the two yarn directions make — a diamond that is square means the yarns cross at right angles, which is the 45° case. For shop-floor inspection the visual read is normally enough: the angle is either the one on the approved sample or it is not.
Diameter. Measure it, do not assume it. The diameter is half the braid angle calculation, and a braid that closes to a different diameter than expected will show a different angle at an unchanged setting.
What Each Deviation Costs
| Deviation | How it appears | What it costs |
|---|---|---|
| Pitch set too long | Uniformly open braid for the whole run; visible gaps between yarns; braid angle flatter than the approved sample | Failed appearance check against GB/T 3003-2006; poor sealing in service; lower tensile per unit length despite correct yarn |
| Pitch set too short | Hard, over-packed surface; braid stiff and difficult to bend; yarn consumption above the quoted figure | Material cost per metre rises; flexibility and handling suffer; increased abrasion and break-stop trips at the braiding point |
| Density changed without changing carrier count | Coverage corrected by speed alone, with too few yarn ends to close the surface | The braid can never reach the required cover factor however short the pitch is made |
| Same setting reused across a diameter change | Angle wrong on one of the two sizes, though pitch is correct on both | The customer receives a product that does not match the approved sample; sealing behaviour differs from the tested article |
Three of those four rows are set-up errors rather than running errors, and all four are prevented the same way: the process parameter record is filled in before the run and kept afterwards. A parameter without a recorded source is a parameter nobody can defend when a customer, an auditor or the next shift asks where it came from. (field practice)
Where the Setting Sits in the Line
Pitch and braid angle are set after threading and before braiding, which means they are the first settings that assume the yarn path is already correct. A yarn that missed the tension drop-weight, or that was routed backwards around a guide roller, will not hold the pitch it was set to, however accurately the take-up was dialled in — that failure mode belongs to the yarn tension article in this series. And changing the yarn specification or the carrier count changes the pitch that the product needs, which is a changeover rather than a speed adjustment.
The measured numbers on a finished roll — pitch, angle and diameter — are also the three quantities that make a defect traceable. Density along the whole length is a pitch answer; a pattern that repeats once per revolution is a deck answer (see the braid structure article); missing yarn ends are a yarn answer. Keeping those apart is the fastest route from a rejected roll back to the setting that caused it.
Frequently Asked Questions
What is pitch in ceramic fiber braiding?
Pitch is the axial distance the braid advances during one interlacement cycle — one pass in which the carriers cross at the braiding point. It is set by the ratio of the two speeds the machine runs at: pitch equals haul-off or take-up speed divided by interlacement cycles per minute. It is not a property of the yarn or of the deck, which is why a process card lists spindle speed and haul-off speed as a pair rather than separately.
What is braid angle and how is it set?
The braid angle is the angle between a yarn and the axis of the braid. It is set indirectly: the operator sets pitch, and the angle follows from pitch and the product circumference. A yarn wrapping the tube once covers the circumference, 2πR, while the braid advances by the lead, so tan α equals circumference divided by lead. For a given machine and construction, lead and pitch differ only by a constant factor, so shortening the pitch opens the braid angle toward the transverse and lengthening it lays the yarns closer to the axis. A closed braid angle on finished packing sits close to 45°, where lead equals circumference.
Why does the same machine setting give a different braid angle on a thicker rope?
Because the angle depends on the circumference as well as the pitch. Lead is fixed by the take-up and the carrier motion, so at a fixed setting a larger braid has a larger circumference and tan α rises — the angle opens toward the transverse. Setting up on a small diameter and then running a large one without changing the process card does not reproduce the approved braid; it reproduces the same pitch on a bigger circumference, which is a different braid. To hold the angle constant across a diameter change, the lead has to change in proportion to the diameter, which means the take-up has to change with it.
How do I measure pitch and braid angle on a finished braid?
Lay a length of braid flat and straight on a lit surface. For pitch, find a feature that repeats — the point at which the diamond pattern returns to the same phase — mark across ten repetitions, measure the span and divide, which removes most of the reading error. For braid angle, place a straight edge along the axis and read the angle of one visible yarn against it, or read the diamond formed by the two yarn directions: a diamond that is square means the yarns cross at right angles, which is the 45° case. Measure the diameter as well rather than assuming it, because it is half of the angle calculation.
What happens if the pitch is set too long or too short?
Too long a pitch spreads the same yarn ends over more length, producing a uniformly open braid for the whole run with visible gaps and a braid angle flatter than the approved sample — it fails the appearance requirements of GB/T 3003-2006 and seals poorly in service. Too short a pitch packs more yarn into every metre, giving a hard, over-packed, stiff braid, higher yarn consumption per metre and more abrasion and break-stop trips at the braiding point. Because the take-up affects every metre equally, a pitch error is always uniform along the run, which is how it is distinguished from a deck or yarn fault.
Can coverage be corrected with pitch alone?
Only up to a point. Coverage depends on both pitch and carrier count: carrier count sets how many yarn ends are available in each interlacement cycle, and pitch sets how much length those cycles are stretched over. If there are too few yarn ends to close the surface, no reduction in pitch will reach the required cover factor — the braid simply becomes over-packed and still open. Coverage has to be designed with both levers together, which is why the process card records carrier count and pitch as one setting rather than as two independent numbers.